Paint keeps peeling off galvanised steel? The problem is the zinc, not the paint
Touching up galvanised steel is the classic field failure: the paint goes on beautifully, passes inspection, and six months later a fingernail lifts a sheet of it. The cause is not the paint but three properties of the zinc surface.
1. Why adhesion is so poor
Smoothness: hot-dip galvanising has almost no profile, so the paint has nothing to key into. Chemical inertness: the oxide layer seals the zinc's reactivity and ordinary resins struggle to bond. Contamination: galvanised steel usually carries protective oil, a passivation film (chromate) and white rust (zinc oxide and hydroxide).
Together that is painting onto a surface that is slippery, oily and inert. Miss any one and adhesion will not hold.
2. Surface preparation is the only reliable answer
The standard method is sweep blasting: low pressure with a non-metallic abrasive such as garnet, dulling the gloss and removing oxide and contamination without destroying the zinc. It is the most reliable approach in industry.
Where blasting is impossible, a dedicated galvanised-steel treatment — usually a mildly acidic conversion solution or a molybdates wash primer — forms a conversion film to bridge. Less consistent than sweep blasting but adequate for maintenance.
Never: strong acid pickling, aggressive wire brushing that breaks the zinc locally into pitting, or coating over a surface that has not been degreased.
3. Paint selection has a clear preference
Epoxy first — epoxy primer, MIO epoxy, epoxy topcoat — because epoxy wets metal well and shrinks less. Polyurethane second, as a topcoat, with good weathering but adhesion dependent on the primer.
Alkyd and oil-based paints are not recommended. Alkyd saponifies on zinc: the zinc reacts with the resin's acid groups to form zinc soap and the film peels from the interface. It is the commonest wrong choice and fails within about six months.
4. Two easily missed details
Passivation. New galvanising often carries a chromate passivation that makes the surface more inert. A water drop beading and rolling off indicates a film; treatment or light sweeping removes it.
White rust. Galvanised steel stored damp grows a white powdery corrosion product that is loose and weak. It must come off down to dense zinc, or the paint simply adheres to white rust.