Epoxy will dry at 5 °C — but dry is not cured
Epoxy curing is a chemical reaction and reaction rate is extremely temperature-sensitive. The rule of thumb is that cure time roughly doubles for every 10 °C drop — and below 10 °C it gets worse than that, because some hardeners almost stop reacting.
1. Why it looks dry
Physical drying of solvent or part of the resin removes surface tack while crosslinking is still incomplete. It feels dry to the finger but dents under a nail, or wipes off with solvent. That is false dryness.
The problems appear later: the next coat lifts it, pull-off adhesion is low, chemical resistance misses the specification. The difficulty is that none of this is visible on the day.
2. Three temperature thresholds
10 °C is the practical floor for standard epoxy; below that cure slows markedly and needs extended curing or heat. 5 °C is the absolute floor for most products — below it the reaction essentially stops and the work is wasted.
One limit is commonly missed: substrate temperature, not air temperature. On a winter morning steel can be 5 °C or more below air temperature after night-time radiation, so judging by air temperature misleads. Measure the steel.
3. Four responses to cold weather
Switch system: use a low-temperature or winter-grade product whose hardener is modified to react at 5 °C, at the cost of shorter pot life and darker colour. Apply heat: blowers, infrared or a temporary shelter to bring the substrate above 10 °C and hold it until cure completes — hold it, not just during application.
Extend intervals, re-planning the schedule against the maker's cold-cure curve rather than warm-weather habit. And reduce per-coat thickness, since a thin film dissipates reaction heat less and cures more evenly.
4. Confirming it really cured
Do not rely on a finger. Three workable checks: solvent rub (MEK or acetone, 50 double rubs without softening), coin scratch (no soft mark), and the most reliable — glass transition temperature or a pull-off test.
Without instruments, a parallel test panel is the practical route: same temperature, same DFT, cured alongside the structure, then used for destructive testing. That panel is worth far more than any judgement by feel.