Why inorganic zinc will not cure in dry weather: it needs moisture from the air
The commonest complaint about inorganic zinc (ethyl silicate type) in a shop is 'it still wipes off a day later'. Check the record: 25 °C, 35% RH, beautiful weather. That is the problem — too beautiful.
1. A completely different curing mechanism
Epoxy crosslinks chemically and moisture is the enemy, which is why epoxy application limits humidity. Ethyl silicate inorganic zinc is the opposite: it hydrolyses by absorbing moisture from the air to form silicic acid, which then reacts with the zinc and the steel surface to build the film. Without water the reaction barely proceeds.
That explains two things: slow cure in dry weather, and the field trick of misting water or covering with damp cloth to accelerate it. The trick applies only to ethyl silicate, not to lithium silicate — that one cures by losing its own water and moisture actually harms it. Confirm which type before ordering.
2. Where the humidity window sits
The practical window for ethyl silicate is 50–85% RH at 10–35 °C. Below 50% cure slows markedly, below 30% it effectively stops. Above 85%, or with steel close to dew point, the surface condenses, which whitens the film and drops adhesion.
So a summer shop and a heated winter shop are two different problems: the rainy season is too humid, a heated northern shop in winter is too dry. The first needs dehumidification, the second humidification — which sounds absurd until you have to do it.
3. Three consequences of under-cure
First, the next coat lifts it: an incompletely cured silicate network re-dissolves in the intermediate's solvent, causing lifting and wrinkling. Second, adhesion is short — pull-off values at about half. Third, salt spray performance is nowhere near the design figure, because the film is not yet dense.
A rough field check: rub hard with a water-dampened white cloth; no colour on the cloth means essentially cured. Formal judgement follows the maker's cure time and conditions, or a MEK rub test.
4. Three hard requirements
Preparation to Sa2.5 with 50–75 µm profile — inorganic zinc bonds by both mechanical keying and chemical reaction, and a shallow profile lets the whole film peel. Continuous agitation, because zinc settles very fast and a pause mid-spray changes the zinc content between passes. And strict DFT control: 75 µm is typical, and above 125 µm it cracks readily because flexibility is poor.
One more: do not blast air at it straight after spraying. Strong airflow carries surface moisture away and slows cure further. The shop habit of 'putting a fan on it to dry faster' does the opposite.