A coating rated 400 °C on a 400 °C line: right choice? Check continuous versus peak first
The easy route is to match the equipment's maximum temperature against the maker's rating. That fails twice: it treats a peak as continuous, and it assumes temperature resistance is the whole story.
1. How far apart continuous and peak really are
Continuous temperature is steady operating temperature, typically 90% or more of running time. Peak temperature comes from start-up, shutdown, overload or upset conditions — minutes to hours.
Silicone ratings are generally continuous. A short excursion 50 °C above is usually not immediate failure, but each one accelerates resin degradation. Equipment started once a day sees 300 excursions a year; the cumulative effect equals running hot.
2. Cycling damages more than heat
Coating and steel have different expansion coefficients, so a temperature change elongates them differently and generates shear stress at the interface. More cycles mean repeated loading and a gradual loss of adhesion.
This explains a familiar pattern: the same 400 °C silicone lasts eight years on a cracking furnace shell held at temperature, and three years on an exhaust duct started daily. Not a bad paint — a different duty.
3. The medium picks the resin; temperature only sets the ceiling
At the same 300 °C, sulphur-bearing flue gas, chlorine and oxidising atmospheres demand completely different resins. Silicone aluminium resists oxidation but is attacked in reducing sulphur atmospheres, where a ceramic-filled or flue-gas-specific system is needed.
So the order is: fix the medium, then the temperature ceiling, then thickness and system. Reverse it and you readily buy something heat-resistant enough but chemically wrong.
4. Two fatal points in application
Cure. Most silicones do not cure, or cure very slowly, at ambient — the first heat-up does it. Too steep a ramp and solvent and moisture cannot escape, blistering over large areas. Follow the maker's staged curve with holds at critical temperatures.
Thickness. Heat-resistant coatings are usually thin, 25–40 µm per coat; building them thick cracks under cycling. Do not carry over thickness habits from ambient-cure products.