Application

Pinholes and blisters are not the same defect: reading the cause from the shape

The site reports 'blistering'. You arrive and find some defects are pinhead holes and some are coin-sized bumps. Different causes, different repairs, different liability — but both got flattened into one word, so the conversation was wrong from the start.

1. Read the shape, not the size

A pinhole is a small hole through or into the film; it reads as a depression and a fingernail catches the pit. A blister is a bump where the film has separated from the substrate or the coat beneath; it is raised, gives under pressure, and cut open it is hollow or holds liquid.

One action separates them: slice across the defect with a blade. A hole has continuous film with a piece missing; a blister shows a clear cavity and a separation plane. Skip that step and everything after is guessing.

2. Where pinholes come from

Trapped solvent: too thick a coat seals the surface, solvent cannot escape and breaks through. The tell is a cratered rim, with density rising with film thickness.

Substrate outgassing: moisture or gas in concrete, galvanising, or left after blasting escapes through the wet film. The tell is clustering at welds and repair areas.

Spray parameters: gun too far, viscosity too high, poor atomisation — droplets dry in flight and land as non-coalescing particles and holes. The tell is even distribution across the whole area.

Entrained air: applied without a settling period after mixing, or air whipped in during two-pack mixing. The tell is smooth-walled, larger holes.

3. Where blisters come from

Osmotic blistering: water crosses the film, dissolves residual salts or water-soluble material at the interface, and keeps diffusing in to lift the film. The tell is liquid inside, saline or conductive, concentrated in wet or humid areas. This is the dangerous one — strip and recoat without removing the salt and it returns.

Cathodic disbondment: a galvanic couple at a defect on zinc-rich primer or steel creates alkali that destroys interfacial adhesion and spreads outward. The tell is blisters strung along a scribe or weld.

Residual intercoat solvent: recoated too soon, the lower coat's solvent is sealed in and slowly lifts the film. The tell is large soft blisters appearing days to weeks after recoating.

4. How the repairs differ

Pinholes: solvent-trapping type, abrade the whole area until no holes remain and recoat; parameter type, correct the parameters and respray the area. Spot-filling pinholes rarely works — the hole goes through, and a surface patch does not close the channel.

Blisters: osmotic type must be stripped to substrate, salt removed completely, surface re-prepared and the system rebuilt. Cathodic type needs removal extending at least 50 mm beyond the visible blister edge. Intercoat type is stripped to the lower coat, dried fully and redone.

One shared diagnostic: look at the interface. Clean separation points to adhesion or stress; rust, salt or water at the interface means osmosis or cathodic disbondment.

5. Preventing the next batch

Keep each coat within the maker's maximum — two coats rather than one. Test for salt after blasting, especially coastal work and overcoating old systems. Confirm the recoat interval and abrade if it is overrun. Let mixed material stand 5–10 minutes before use.

Those four eliminate most pinholes and blisters. What remains is usually a material-to-substrate mismatch — which is a selection problem, not an application one.