Application

Sa2.5 is not the finish line: why you still test for salt

Blasting acceptance checks two things: cleanliness and profile. Most projects stop there. Coastal work, overcoating old systems, and demanding locations such as ballast tanks need a third — soluble salt.

1. Where the salt comes from

Three sources. Marine environment: sea breeze deposits salt on steel, including plate shipped from overseas and stored inland. Old coatings: aged paint absorbs salt in service, blasting removes the paint but the salt has entered the surface pits. And the abrasive itself: sea sand or contaminated media drives salt straight into the surface.

The second is most often missed. On a ship ten years in service, ballast tank internals can carry tens of milligrams of salt per square metre, and it is still in the pits after blasting to Sa2.5.

2. How salt destroys a coating

The mechanism is osmosis. Salt under the film dissolves in water that permeates in, forming a concentrated solution, and surrounding water keeps diffusing inward to lift the film into blisters. No defect is needed — water molecules pass through any organic coating.

So on high-salt substrate, even with perfect application and correct DFT, dense blistering appears within months to two years. Cut them open and there is rust and salt crystal at the base. This is why such failures get misdiagnosed as a paint quality problem.

3. Standards and method

Common limits follow ISO 8502-6/-9: 50 mg/m² or less in general atmosphere, 20 mg/m² for immersion and severe marine, stricter under PSPC for ballast tanks. Methods are the Bresle patch (inject pure water, extract, measure conductivity) and conductivity pens — the first is more accurate, the second faster.

Bresle technique: press the patch flat with no bubbles, inject water in proportion to patch area (typically 3 ml per 12.5 cm²), and wait at least four minutes before extracting so the salt dissolves. Skipping the wait is the commonest error, and it reads low — which is more dangerous, not less.

4. What to do when it fails

Re-blasting does not fix it — that only pushes salt deeper. The correct response is high-pressure fresh water washing (at least 10 MPa, with wash water lower in salt than the surface being washed), then drying and re-testing.

If repeated washing still fails, the salt has entered deep pitting in the steel and plate replacement has to be considered. In ballast tanks, forcing a coating on means redoing the whole tank a few years later.

5. When testing is mandatory

Any one of four conditions: work within 10 km of the coast; refurbishing old steel that served in a marine environment; ballast, potable water or cargo oil tank internals; and C5 or CX systems with a design life beyond 15 years.

Sample density by area, typically no fewer than three points per 100 m², with extra points at welds and edges. Keep the records — in a blistering dispute they are the only evidence that the work complied.

Need selection advice?

Tell us your substrate and service conditions

One-to-one coating consultancy: system design, quantity take-off and quotation.