Tank linings: produce the medium list before discussing resin
The first step in lining selection is not the catalogue, it is a form the owner or process engineer fills in: medium, concentration, temperature, whether exposures alternate, and whether solids are present. Without that form, every later discussion is guesswork.
1. Four typical media, four resin families
Ambient dilute acid, dilute alkali, brine: bisphenol-A epoxy or epoxy bitumen is enough — low cost, forgiving application. The commonest case and the easiest to get right.
Concentrated and oxidising acids (nitric, chromic), mixed acids: phenolic epoxy or vinyl ester. Vinyl ester handles oxidising acid better, at higher cost and greater shrinkage.
Organic solvents (aromatics, ketones, esters): standard epoxy swells; phenolic epoxy, vinyl ester or a thermoplastic lining such as PVDF is needed. Failure here shows as softening and blistering rather than corrosion.
Hot media above 80 °C: the resin options narrow sharply and thermal cycling must be considered. Phenolic epoxy reaches around 120 °C; beyond that needs special systems or inorganic lining.
2. Alternating exposure is the most commonly missed condition
One tank may hold different media in turn — diesel then petrol, or acid then alkali. Resistance data for a single medium does not transfer to alternating duty, because residue reacts with the incoming medium.
For alternating service you need the full list and the switching frequency, and the resin must be selected for the worst combination. Skip that question and selection becomes a gamble.
3. Thicker is not safer
Lining thickness is typically 300–500 µm in two or three coats. Too thick and cure shrinkage stress cracks it; too thin and the barrier is insufficient. What matters is total thickness matched to coat count, with each coat properly cured.
One counter-intuitive fact: multiple thin coats usually beat one thick coat chemically, because the intercoat interfaces interrupt permeation paths, while defects inside a single thick coat run right through.
4. Acceptance fails more often than selection
Three checks: thickness, holiday testing at 100% coverage with no sampling, and degree of cure. Holiday testing is the only way to find pinholes, and one pinhole in a lining means the medium reaches the steel directly.
Cure testing is often skipped and is a leading cause of failure. Incompletely cured phenolic epoxy and vinyl ester look normal and read acceptably hard, then soften within days of contact. Use a Barcol hardness tester or a solvent rub on site.