Interdur 8802
Interdur 8802 is a MIO epoxy intermediate from AkzoNobel. This page groups model identity, system position and the data request entry so you can verify the full system before enquiring.
Key technical data
| Volume solids | 67% |
|---|---|
| Dry film thickness | 75–100 µm (3–4 mils) |
| Theoretical spreading rate | 8.93 m²/L |
| VOC | 2.64 lb/gal (317 g/L) US EPA Method 24 |
| Density / specific gravity | 1.54 kg/L (12.9 lb/gal) |
| Number of components | Two-component |
| Thinner | International GTA220 |
| Mixing ratio | 3 parts: 1 part (by volume) |
The technical content below is reproduced in English as published by the manufacturer; terms, grades and values follow the English original.
How this coating class protects
Micaceous iron oxide is a lamellar pigment. During application the flakes stack in layers and turn the path of water, oxygen and ions into a long, tortuous route. The value is not one more coat; it is that this coat separates the coats above and below while plugging pinholes and micro-defects. High build is its advantage over a topcoat.
What to verify in the original TDS
These are checking criteria, not numeric commitments. Every figure follows the current original TDS.
- Lamellar pigment content and flake sizeMIO loading drives barrier efficiency. A low-loaded product is essentially a coloured epoxy with an order of magnitude less barrier performance.
- Maximum DFT in a single coatHigh build is the whole point. If the data sheet caps single-coat thickness low, the formulation struggles with sagging or cracking and you will need multiple coats, which changes both schedule and cost.
- Overcoating windows to primer and topcoatIntermediate coats present a large exposed area for a long time; past the window they must be abraded. Window length drives the sequence plan.
- Presence of zinc or conductive filler for zinc-rich systemsOver a zinc-rich primer, a non-conductive intermediate cuts the cathodic protection path. This detail is easily missed in cross-brand systems.
Application control points
High build does not mean brushing it thick
Thick films need airless spray, the right tip and controlled pass speed. Rollering a thick film gives you a dry skin over uncured material, which then shrinks and cracks.
Stripe coat welds and edges first
The barrier value of an intermediate is most easily wasted at edges. Stripe coating before the full pass gets the edge thickness right.
Overcoating before full cure traps solvent
A thick intermediate releases solvent slowly. Topcoating at touch-dry seals solvent inside and blisters appear months later. Work to the hard-dry time in the TDS, not to the feel of the surface.
How to settle site disputes
Using the intermediate as filler
It is not a body filler. Using it to fill pits and weld spatter pushes local thickness far past design and concentrates cracking risk there. Substrate flatness belongs to the substrate stage.
Ignoring the conductive path in cross-brand systems
Zinc-rich primer plus another brand's intermediate, where the intermediate is a strong barrier without conductive filler, cuts the reach of cathodic protection. Inspection will not show it; the corrosion pattern years later will.
Common questions on this coating class
Can the intermediate coat be dropped?
MIO intermediate versus plain epoxy intermediate?
The above gives class-level technical requirements and judging methods. Specific values and systems follow the current original TDS and the project specification.
Place in the coating system
Typically used as an intermediate build coat adding barrier and total DFT; a topcoat is still required.